HEATS 发表于 2010-9-12 17:00:51

各种材料拉深时的单位压边力数据

<DIV id=NewsContentLabel class=NewsContent><SPAN class=blk14>在单动-压力机</A>上拉深时的单位压边力
<P></P></SPAN>
<DIV align=center>
<CENTER>
<TABLE class=table1 border=1 cellSpacing=0 borderColor=#b5dba2 cellPadding=2 width="80%" height=150>
<TBODY>
<TR bgColor=#e9fde4>
<TD width=317>
<DIV align=center>材&nbsp;&nbsp;&nbsp;&nbsp; 料</DIV></TD>
<TD width=331>
<DIV align=center>q/MPa</DIV></TD></TR>
<TR>
<TD width=317>
<DIV align=center>铝</DIV></TD>
<TD width=331>
<DIV align=center>0.8~1.2</DIV></TD></TR>
<TR>
<TD width=317>
<DIV align=center>紫铜,杜拉铝(退火的或刚淬火的)</DIV></TD>
<TD width=331>
<DIV align=center>1.2~1.8</DIV></TD></TR>
<TR>
<TD width=317>
<DIV align=center>黄铜</DIV></TD>
<TD width=331>
<DIV align=center>1.5~2.0</DIV></TD></TR>
<TR>
<TD width=317>
<DIV align=center>压轧青铜</DIV></TD>
<TD width=331>
<DIV align=center>2.0~2.5</DIV></TD></TR>
<TR>
<TD width=317>
<DIV align=center>20钢、08钢、镀锡钢板</DIV></TD>
<TD width=331>
<DIV align=center>2.5~3.0</DIV></TD></TR>
<TR>
<TD width=317>
<DIV align=center>软化耐热钢</DIV></TD>
<TD width=331>
<DIV align=center>2.8~3.5</DIV></TD></TR>
<TR>
<TD width=317>
<DIV align=center>高合金钢,高锰钢,不锈钢</DIV></TD>
<TD width=331>
<DIV align=center>3.0~4.5</DIV></TD></TR></TBODY></TABLE></CENTER></DIV><BR>
<DIV align=center><SPAN class=blk14>在双动压力机上拉深时的单位压边力</SPAN>
<P></P></DIV>
<DIV align=center>
<CENTER>
<TABLE class=table1 border=1 cellSpacing=0 borderColor=#b5dba2 cellPadding=2 width="80%">
<TBODY>
<TR bgColor=#e9fde4>
<TD width="49%">
<DIV align=center>工件复杂程度</DIV></TD>
<TD width="51%">
<DIV align=center>q/MPa</DIV></TD></TR>
<TR>
<TD width="49%">
<DIV align=center>难加工件</DIV></TD>
<TD width="51%">
<DIV align=center>3.7</DIV></TD></TR>
<TR>
<TD width="49%">
<DIV align=center>普通加工件</DIV></TD>
<TD width="51%">
<DIV align=center>3.0</DIV></TD></TR>
<TR>
<TD width="49%">
<DIV align=center>易加工件</DIV></TD>
<TD width="51%">
<DIV align=center>2.5</DIV></TD></TR></TBODY></TABLE></CENTER></DIV>
<TABLE class=table1 border=1 cellSpacing=0 borderColor=#b5dba2 cellPadding=2 width="80%">
<TBODY>
<TR bgColor=#e9fde4>
<TD width="52%">
<DIV align=center>材&nbsp;&nbsp;&nbsp; 料</DIV></TD>
<TD width="48%">
<DIV align=center>单位压边力q/MPa</DIV></TD></TR>
<TR>
<TD width="52%">
<DIV align=center>铝(退火状态)</DIV></TD>
<TD width="48%">
<DIV align=center>0.8~1.2</DIV></TD></TR>
<TR>
<TD width="52%">
<DIV align=center>铝(硬态)</DIV></TD>
<TD width="48%">
<DIV align=center>1.2~1.4</DIV></TD></TR>
<TR>
<TD width="52%">
<DIV align=center>黄铜(退火状态)</DIV></TD>
<TD width="48%">
<DIV align=center>1.5~2.0</DIV></TD></TR>
<TR>
<TD width="52%">
<DIV align=center>黄铜(硬态)</DIV></TD>
<TD width="48%">
<DIV align=center>2.4~2.6</DIV></TD></TR>
<TR>
<TD width="52%">
<DIV align=center>铜(退火状态)</DIV></TD>
<TD width="48%">
<DIV align=center>1.2~1.8</DIV></TD></TR>
<TR>
<TD width="52%">
<DIV align=center>铜(硬态)</DIV></TD>
<TD width="48%">
<DIV align=center>1.8~2.2</DIV></TD></TR>
<TR>
<TD width="52%">
<DIV align=center>康铜BMn40-1.5(硬态)</DIV></TD>
<TD width="48%">
<DIV align=center>2.6~2.9</DIV></TD></TR>
<TR>
<TD width="52%">
<DIV align=center>可伐合金4J29(退火状态)</DIV></TD>
<TD width="48%">
<DIV align=center>3.0~3.3</DIV></TD></TR>
<TR>
<TD width="52%">
<DIV align=center>钼(退火状态)</DIV></TD>
<TD width="48%">
<DIV align=center>4.0~4.5</DIV></TD></TR>
<TR>
<TD width="52%">
<DIV align=center>软钢t<0.5mm</DIV></TD>
<TD width="48%">
<DIV align=center>2.5~3.0</DIV></TD></TR>
<TR>
<TD width="52%">
<DIV align=center>软钢t>0.5mm</DIV></TD>
<TD width="48%">
<DIV align=center>2.0~2.5</DIV></TD></TR>
<TR>
<TD width="52%">
<DIV align=center>不锈钢1Cr18Ni9Ti</DIV></TD>
<TD width="48%">
<DIV align=center>4.5~5.5</DIV></TD></TR>
<TR>
<TD width="52%">
<DIV align=center>镍铬合金Cr20Ni80</DIV></TD>
<TD width="48%">
<DIV align=center>3.5~4.0</DIV></TD></TR></TBODY></TABLE></DIV>
               